Clad plate is ordered to one of four ASME/ASTM product specifications, and the cladding alloy decides which one: SA-263 for stainless chromium steels (such as 410S), SA-264 for stainless chromium-nickel steels including duplex (such as 316L or 2205), SA-265 for nickel and nickel-base alloys (such as 625, 825 or C-276), and SB-898 for reactive and refractory metals (titanium, zirconium, tantalum, niobium). The first three are almost identical in structure; SB-898 has its own rules for testing and bond quality. The ASME versions (SA-/SB-) are identical to the ASTM versions (A263, A264, A265, B898) and are the ones used for ASME Code pressure vessels.
The four standards at a glance
| SA-263 / A263 | SA-264 / A264 | SA-265 / A265 | SB-898 / B898 | |
|---|---|---|---|---|
| Cladding | Stainless chromium steel (ferritic/martensitic) | Stainless chromium-nickel steel, incl. duplex | Nickel and nickel-base alloys | Reactive and refractory metals |
| Typical alloys | 410S, 405, 430 | 304L, 316L, 321, 347, 904L, 2205, 2507 | Nickel 200/201, 400, 600, 625, 825, C-276, C-22 | Titanium Gr. 1, 2, 7, 11, 12; zirconium 700 and 702; tantalum; niobium |
| Base metal | Carbon or low-alloy steel | Carbon or low-alloy steel | Carbon or low-alloy steel | Carbon or low-alloy steel, other bases by agreement |
| Bond shear strength | Min. 140 MPa (20 ksi) when the shear test applies | Min. 140 MPa (20 ksi) when the shear test applies | Min. 140 MPa (20 ksi) when the shear test applies | Min. 137.9 MPa (20 ksi) for titanium; see specification for other metals |
| Ultrasonic bond inspection | Plates ≥ 10 mm per A578 methods; Class 1, 3 or 5 | Plates ≥ 10 mm per A578 methods; Class 1, 3 or 5 | Plates ≥ 10 mm per A578 methods; Class 1, 3 or 5 | Own UT requirements and acceptance limits |
| Shockwave article | n/a | Stainless steel clad plate | ASME SA-265 explained | Titanium clad plate |
What SA-263, SA-264 and SA-265 have in common
- Bond: the cladding must be integrally and continuously bonded to the base, by any process that achieves this, explosion welding, roll bonding or other.
- Base steel: tested to its own specification, for example SA516 Gr. 60/70, SA387 or P265GH / P355GH.
- Cladding: must meet the chemistry of its own ASTM/ASME product specification (for example B443 for Alloy 625 or A240 for 316L).
- Bond tests: a shear test with a minimum of 140 MPa (20 ksi), or bend tests as an alternative where agreed.
- Ultrasonic classes: Class 1 (largest unbonded area 25 mm, total ≤ 1%), Class 3 (75 mm, ≤ 3%) and Class 5 (58 cm², ≤ 5%); if no class is stated, Class 5 may be supplied. See ASTM A578 ultrasonic testing.
- Supplementary requirements: options such as 100% ultrasonic scanning and tests after simulated post-weld heat treatment are ordered separately.
What is different in SB-898
Titanium, zirconium and tantalum cannot be fusion-welded to steel or roll-bonded in a practical way, so reactive-metal clad plate is made almost exclusively by explosion welding. SB-898 reflects this: bond shear testing is a standard requirement for every plate, and the ultrasonic acceptance criteria and the rules for repairs are specific to reactive metals. Post-weld heat treatment is limited in temperature and time, because titanium and zirconium react with steel at high temperature. More in titanium clad plate.
Which standard should you order to?
| Your cladding alloy | Order to |
|---|---|
| 410S, 405 or other chromium stainless | ASME SA-263 |
| 304L, 316L, 317L, 321, 347, 904L | ASME SA-264 |
| Duplex 2205, super duplex 2507 | ASME SA-264 |
| Nickel 200/201, Alloy 400, 600, 625, 825, C-276, C-22 | ASME SA-265 |
| Titanium, zirconium, tantalum, niobium | ASME SB-898 |
| Copper, cupronickel, aluminium | No dedicated ASME product standard, customer specification, with test requirements taken from the closest standard |
Outside ASME projects the same specifications are widely used as the reference, combined with the customer’s technical delivery conditions and, in Europe, the design and material rules of EN 13445 or AD 2000.
What to put on the purchase order
- Clad plate specification and edition, for example ASME SA-264.
- Base steel grade and specification, cladding alloy and specification.
- Base and cladding thicknesses (minimum or nominal), plate size or drawing.
- Ultrasonic quality class and coverage (for example Class 1, 100% scan).
- Bond tests (shear, bend), and tests after simulated PWHT if the vessel will be heat treated, see PWHT of clad plates.
- Certificate type (EN 10204 3.1 or 3.2) and third-party inspection.
Shockwave produces clad plates to all four specifications, with clad layers from 1 to 50 mm and plates up to 60 m² and 50 metric tonnes, and every plate is 100% ultrasonically scanned. See our certifications and documents, the material combinations, or send your specification through our contact page.
Frequently asked questions
What is the difference between SA-263, SA-264 and SA-265?
The cladding alloy. SA-263 covers stainless chromium steels such as 410S, SA-264 covers stainless chromium-nickel steels including duplex, and SA-265 covers nickel and nickel-base alloys. Their test and bond-quality rules are almost the same.
Which standard covers titanium clad plate?
ASME SB-898 (ASTM B898), the specification for reactive and refractory metal clad plate: titanium, zirconium, tantalum and niobium.
What bond shear strength do clad plate standards require?
SA-263, SA-264 and SA-265 require at least 140 MPa (20 ksi) when the shear test applies. SB-898 requires at least 137.9 MPa (20 ksi) for titanium clad plate.
Are ASME SA-264 and ASTM A264 the same?
Yes. ASME adopts the ASTM specification, so SA-264 and A264 have the same technical content. The SA- version is used for ASME Code pressure vessels.
Which standard applies to duplex clad plate?
ASME SA-264, which covers stainless chromium-nickel steels including duplex 2205 and super duplex 2507.
Written by Joeri Hofstede, CEO of Shockwave Metalworking Technologies, vacuum explosion welding specialists since 1985.