{"id":5843,"date":"2026-11-04T09:32:58","date_gmt":"2026-11-04T08:32:58","guid":{"rendered":"https:\/\/shockwave-clad.com\/?p=5843"},"modified":"2026-11-04T09:32:58","modified_gmt":"2026-11-04T08:32:58","slug":"astm-a578-ultraschallpruefung-plattierte-bleche","status":"publish","type":"post","link":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/","title":{"rendered":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung von Blechen und plattierten Blechen"},"content":{"rendered":"<p>[et_pb_section fb_built=&#8220;1&#8243; _builder_version=&#8220;4.27.4&#8243; global_colors_info=&#8220;{}&#8220;][et_pb_row _builder_version=&#8220;4.27.4&#8243; global_colors_info=&#8220;{}&#8220;][et_pb_column type=&#8220;4_4&#8243; _builder_version=&#8220;4.27.4&#8243; global_colors_info=&#8220;{}&#8220;][et_pb_text _builder_version=&#8220;4.27.4&#8243; global_colors_info=&#8220;{}&#8220;]<\/p>\n<p><strong>ASTM A578 (ASME SA-578) ist die Norm f\u00fcr die Ultraschallpr\u00fcfung von gewalzten Blechen aus unlegiertem und legiertem Stahl ab 10 mm (3\/8 in) mit Senkrechteinschallung im Impuls-Echo-Verfahren. Sie findet innere Fehler parallel zur Oberfl\u00e4che \u2013 Dopplungen und bei plattierten Blechen ungebundene Bereiche der Auflage \u2013 und definiert drei Zul\u00e4ssigkeitsstufen: A, B und C.<\/strong> Die Spezifikationen f\u00fcr plattierte Bleche ASME SA-263, SA-264 und SA-265 verweisen f\u00fcr die Pr\u00fcfung der Bindung auf sie, deshalb steht A578 in fast jeder Bestellung plattierter Bleche.<\/p>\n<h2>Geltungsbereich der Norm<\/h2>\n<ul>\n<li><strong>Verfahren:<\/strong> Senkrechteinschallung (0\u00b0) im Impuls-Echo-Verfahren, Kontakt- oder Tauchtechnik.<\/li>\n<li><strong>Werkstoff:<\/strong> gewalzte Bleche aus unlegiertem und legiertem Stahl ab 10 mm (3\/8 in).<\/li>\n<li><strong>Was sie findet:<\/strong> Fehler parallel zu den Walzoberfl\u00e4chen, etwa Dopplungen oder eine ungebundene Plattierungsgrenzfl\u00e4che.<\/li>\n<li><strong>Standardstufe:<\/strong> Stufe B, sofern Besteller und Hersteller nichts anderes vereinbaren.<\/li>\n<\/ul>\n<h2>Pr\u00fcftechnik und Pr\u00fcfraster<\/h2>\n<p>Der Pr\u00fcfkopf hat 25 oder 30 mm (1 oder 1\u215b in) Durchmesser oder ist 25 mm quadratisch; Phased-Array-Systeme sind mit gleichwertiger aktiver Apertur zul\u00e4ssig. Empfohlen wird eine Nennfrequenz von 2,25 MHz, bei Blechen unter 20 mm k\u00f6nnen 5 MHz n\u00f6tig sein. Das Ger\u00e4t wird so eingestellt, dass das erste R\u00fcckwandecho in einem fehlerfreien Bereich 50\u201390 % der Bildschirmh\u00f6he erreicht.<\/p>\n<table style=\"width:100%;border-collapse:collapse;margin-bottom:25px\">\n<tr>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Pr\u00fcfoption<\/th>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Raster<\/th>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">Gitterraster<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Durchgehende senkrecht zueinander verlaufende Linien im Nennabstand von 225 mm (9 in)<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">Querspuren<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Durchgehende parallele Spuren quer zur Blechhauptachse im Abstand von 100 mm (4 in)<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">L\u00e4ngsspuren<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Durchgehende parallele Spuren entlang der Hauptachse im Abstand von 75 mm (3 in) oder weniger<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">R\u00e4nder<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Eine zus\u00e4tzliche Spur innerhalb von 50 mm (2 in) zu allen Blechr\u00e4ndern<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">100 % Abdeckung<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Zusatzanforderung S1 \u2013 l\u00fcckenlose Pr\u00fcfung der gesamten Oberfl\u00e4che<\/td>\n<\/tr>\n<\/table>\n<h2>Was registriert wird<\/h2>\n<ul>\n<li>Jede Anzeige mit <strong>vollst\u00e4ndigem Verlust des R\u00fcckwandechos<\/strong>.<\/li>\n<li>Bei Blechen ab 20 mm (3\/4 in): jede Anzeige von mindestens 50 % des ersten R\u00fcckwandechos, die mit einem R\u00fcckwandechoverlust von 50 % einhergeht.<\/li>\n<li>Wird auf einer Rasterlinie eine registrierpflichtige Anzeige gefunden, wird der umgebende Bereich gepr\u00fcft und die Grenze markiert, an der R\u00fcckwandecho und Anzeige gleich hoch sind.<\/li>\n<\/ul>\n<h2>Zul\u00e4ssigkeitsstufen A, B und C<\/h2>\n<table style=\"width:100%;border-collapse:collapse;margin-bottom:25px\">\n<tr>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Stufe<\/th>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Unzul\u00e4ssig, wenn<\/th>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Typischer Einsatz<\/th>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">A<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Ein durchgehender vollst\u00e4ndiger R\u00fcckwandechoverlust mit Anzeigen in derselben Ebene, der nicht in einen Kreis von 75 mm (3 in) oder der halben Blechdicke \u2013 der gr\u00f6\u00dfere Wert \u2013 passt<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Allgemeine Blechqualit\u00e4t<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">B (Standard)<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Wie Stufe A und zus\u00e4tzlich zwei oder mehr kleinere Fehler, deren Abstand kleiner ist als der Durchmesser des gr\u00f6\u00dferen<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Standard, wenn keine Stufe angegeben ist<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">C<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">Ein durchgehender vollst\u00e4ndiger R\u00fcckwandechoverlust in derselben Ebene, der nicht in einen Kreis von 25 mm (1 in) passt<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">H\u00f6chste Anforderungen<\/td>\n<\/tr>\n<\/table>\n<p>Die Zusatzanforderung S2 versch\u00e4rft die Regeln f\u00fcr eng beieinanderliegende Anzeigen, S4 verlangt eine Konformit\u00e4tsbescheinigung und S8 erg\u00e4nzt die Justierung mit Flachbodenbohrungen f\u00fcr Bleche ab 100 mm (4 in).<\/p>\n<h2>A578 und plattierte Bleche<\/h2>\n<p>Bei plattierten Blechen wird die Bindung nach der jeweiligen Spezifikation bewertet. ASME SA-263 (Chromst\u00e4hle), <a href=\"https:\/\/shockwave-clad.com\/de\/edelstahlplattiertes-blech\/\">SA-264<\/a> (austenitischer Edelstahl und Duplex) und <a href=\"https:\/\/shockwave-clad.com\/de\/asme-sa-265-nickelplattierte-bleche\/\">SA-265<\/a> (Nickellegierungen) verlangen f\u00fcr Bleche ab 10 mm eine Ultraschallpr\u00fcfung nach den Verfahren der A578 und definieren die Bindungsklassen:<\/p>\n<table style=\"width:100%;border-collapse:collapse;margin-bottom:25px\">\n<tr>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Bindungsklasse<\/th>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Gr\u00f6\u00dfte einzelne ungebundene Fl\u00e4che<\/th>\n<th style=\"border:1px solid #ccc;padding:10px;text-align:left\">Ungebundene Fl\u00e4che gesamt<\/th>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">Klasse 1<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">25 mm (1 in) gr\u00f6\u00dfte Ausdehnung<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">\u2264 1 % der plattierten Fl\u00e4che<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">Klasse 3<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">75 mm (3 in) gr\u00f6\u00dfte Ausdehnung<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">\u2264 3 % der plattierten Fl\u00e4che<\/td>\n<\/tr>\n<tr>\n<td style=\"border:1px solid #ccc;padding:10px\">Klasse 5<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">58 cm\u00b2 (9 in\u00b2)<\/td>\n<td style=\"border:1px solid #ccc;padding:10px\">\u2264 5 % der plattierten Fl\u00e4che<\/td>\n<\/tr>\n<\/table>\n<p>Plattierte Bleche aus reaktiven Metallen \u2013 Titan, Zirkonium, Tantal \u2013 fallen unter ASME SB-898 mit eigenen Ultraschallanforderungen (siehe <a href=\"https:\/\/shockwave-clad.com\/de\/titanplattiertes-blech\/\">titanplattiertes Blech<\/a>). Geben Sie in der Bestellung sowohl die Pr\u00fcfnorm als auch die Klasse an, zum Beispiel \u201eUT nach SA-578, Bindungsklasse 1 nach SA-264, 100 % Abdeckung\u201c.<\/p>\n<h2>So pr\u00fcft Shockwave plattierte Bleche<\/h2>\n<p>Jedes Produktionsblech wird unabh\u00e4ngig von der bestellten Klasse auf 100 % der Bindefl\u00e4che mit automatisierter Phased-Array-Ultraschalltechnik gepr\u00fcft. Grundlage ist eine schriftliche Shockwave-Pr\u00fcfanweisung, qualifiziert nach ASME Section V (Artikel 5 und 23), mit Zul\u00e4ssigkeitskriterien nach ASTM A263, A264, A265, A578, B432 und B898, EN 10160, SEL 072 sowie den DNV- und Lloyd&#8217;s-Register-Regeln f\u00fcr \u00dcbergangsverbindungen. Die Anweisung ist von einem Pr\u00fcfer der Stufe 3 nach ISO 9712 \/ ASNT freigegeben, gepr\u00fcft wird von zertifiziertem Personal der UT-Stufe 2. Die Ergebnisse stehen im Pr\u00fcfzeugnis, Abnahmen durch Dritte sind willkommen.<\/p>\n<p>Siehe unsere <a href=\"https:\/\/shockwave-clad.com\/de\/zertifizierungen-und-dokumentation\/\">Zertifizierungen und Dokumentation<\/a>, das gesamte Programm an <a href=\"https:\/\/shockwave-clad.com\/de\/plattierte-bleche\/\">plattierten Blechen<\/a>, oder senden Sie uns Ihre Spezifikation \u00fcber unsere <a href=\"https:\/\/shockwave-clad.com\/de\/kontakt\/\">Kontaktseite<\/a>.<\/p>\n<h2>H\u00e4ufig gestellte Fragen<\/h2>\n<h3>Was ist ASTM A578?<\/h3>\n<p>ASTM A578 (ASME SA-578) ist die Norm f\u00fcr die Ultraschallpr\u00fcfung gewalzter Bleche aus unlegiertem und legiertem Stahl ab 10 mm mit Senkrechteinschallung im Impuls-Echo-Verfahren. Sie findet Dopplungen und andere Fehler parallel zur Oberfl\u00e4che und definiert die Zul\u00e4ssigkeitsstufen A, B und C.<\/p>\n<h3>Welche Zul\u00e4ssigkeitsstufen hat A578?<\/h3>\n<p>Stufe A lehnt einen durchgehenden vollst\u00e4ndigen R\u00fcckwandechoverlust ab, der nicht in einen Kreis von 75 mm oder der halben Blechdicke passt; Stufe B erg\u00e4nzt eine Regel f\u00fcr eng beieinanderliegende Anzeigen und ist der Standard; Stufe C lehnt jeden solchen Bereich ab, der gr\u00f6\u00dfer als ein Kreis von 25 mm ist.<\/p>\n<h3>Wird A578 f\u00fcr plattierte Bleche verwendet?<\/h3>\n<p>Ja. ASME SA-263, SA-264 und SA-265 verlangen f\u00fcr plattierte Bleche ab 10 mm eine Ultraschallpr\u00fcfung nach den Verfahren der A578; die Bindung wird nach Klasse 1, 3 oder 5 bewertet.<\/p>\n<h3>Verlangt A578 eine 100-%-Pr\u00fcfung?<\/h3>\n<p>Nein. Die Norm pr\u00fcft entlang eines Rasters oder paralleler Spuren; 100 % Abdeckung ist die Zusatzanforderung S1. Shockwave pr\u00fcft standardm\u00e4\u00dfig 100 % der Bindefl\u00e4che jedes plattierten Blechs.<\/p>\n<h3>Welche Frequenz wird f\u00fcr die Pr\u00fcfung nach A578 verwendet?<\/h3>\n<p>Empfohlen wird eine Nennfrequenz von 2,25 MHz; bei Blechen unter 20 mm k\u00f6nnen 5 MHz n\u00f6tig sein.<\/p>\n<p><em>Verfasst von Joeri Hofstede, CEO von Shockwave Metalworking Technologies \u2013 Spezialisten f\u00fcr Vakuum-Sprengschwei\u00dfen seit 1985.<\/em><\/p>\n<p>[\/et_pb_text][et_pb_code _builder_version=&#8220;4.27.4&#8243; global_colors_info=&#8220;{}&#8220;]<script type=\"application\/ld+json\">{\"@context\":\"https:\/\/schema.org\",\"@type\":\"FAQPage\",\"mainEntity\":[{\"@type\":\"Question\",\"name\":\"Was ist ASTM A578?\",\"acceptedAnswer\":{\"@type\":\"Answer\",\"text\":\"ASTM A578 (ASME SA-578) ist die Norm f\u00fcr die Ultraschallpr\u00fcfung gewalzter Bleche aus unlegiertem und legiertem Stahl ab 10 mm mit Senkrechteinschallung im Impuls-Echo-Verfahren. Sie findet Dopplungen und andere Fehler parallel zur Oberfl\u00e4che und definiert die Zul\u00e4ssigkeitsstufen A, B und C.\"}},{\"@type\":\"Question\",\"name\":\"Welche Zul\u00e4ssigkeitsstufen hat A578?\",\"acceptedAnswer\":{\"@type\":\"Answer\",\"text\":\"Stufe A lehnt einen durchgehenden vollst\u00e4ndigen R\u00fcckwandechoverlust ab, der nicht in einen Kreis von 75 mm oder der halben Blechdicke passt; Stufe B erg\u00e4nzt eine Regel f\u00fcr eng beieinanderliegende Anzeigen und ist der Standard; Stufe C lehnt jeden solchen Bereich ab, der gr\u00f6\u00dfer als ein Kreis von 25 mm ist.\"}},{\"@type\":\"Question\",\"name\":\"Wird A578 f\u00fcr plattierte Bleche verwendet?\",\"acceptedAnswer\":{\"@type\":\"Answer\",\"text\":\"Ja. ASME SA-263, SA-264 und SA-265 verlangen f\u00fcr plattierte Bleche ab 10 mm eine Ultraschallpr\u00fcfung nach den Verfahren der A578; die Bindung wird nach Klasse 1, 3 oder 5 bewertet.\"}},{\"@type\":\"Question\",\"name\":\"Verlangt A578 eine 100-%-Pr\u00fcfung?\",\"acceptedAnswer\":{\"@type\":\"Answer\",\"text\":\"Nein. Die Norm pr\u00fcft entlang eines Rasters oder paralleler Spuren; 100 % Abdeckung ist die Zusatzanforderung S1. Shockwave pr\u00fcft standardm\u00e4\u00dfig 100 % der Bindefl\u00e4che jedes plattierten Blechs.\"}},{\"@type\":\"Question\",\"name\":\"Welche Frequenz wird f\u00fcr die Pr\u00fcfung nach A578 verwendet?\",\"acceptedAnswer\":{\"@type\":\"Answer\",\"text\":\"Empfohlen wird eine Nennfrequenz von 2,25 MHz; bei Blechen unter 20 mm k\u00f6nnen 5 MHz n\u00f6tig sein.\"}}]}<\/script>[\/et_pb_code][\/et_pb_column][\/et_pb_row][\/et_pb_section]<\/p>\n","protected":false},"excerpt":{"rendered":"<p>Was ASTM A578 \/ ASME SA-578 f\u00fcr die Ultraschallpr\u00fcfung von Stahlblechen mit Senkrechteinschallung verlangt, ihre Zul\u00e4ssigkeitsstufen und die Anwendung auf plattierte Bleche.<\/p>\n","protected":false},"author":3,"featured_media":5834,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_et_pb_use_builder":"on","_et_pb_old_content":"","_et_gb_content_width":"","footnotes":""},"categories":[53],"tags":[],"class_list":["post-5843","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-technische-bibliothek"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.8 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave<\/title>\n<meta name=\"description\" content=\"ASTM A578 \/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/\" \/>\n<meta property=\"og:locale\" content=\"de_DE\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave\" \/>\n<meta property=\"og:description\" content=\"ASTM A578 \/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/\" \/>\n<meta property=\"og:site_name\" content=\"Shockwave\" \/>\n<meta property=\"article:published_time\" content=\"2026-11-04T08:32:58+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg\" \/>\n\t<meta property=\"og:image:width\" content=\"1600\" \/>\n\t<meta property=\"og:image:height\" content=\"900\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/jpeg\" \/>\n<meta name=\"author\" content=\"Joeri Hofstede\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Verfasst von\" \/>\n\t<meta name=\"twitter:data1\" content=\"Joeri Hofstede\" \/>\n\t<meta name=\"twitter:label2\" content=\"Gesch\u00e4tzte Lesezeit\" \/>\n\t<meta name=\"twitter:data2\" content=\"5\u00a0Minuten\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/\"},\"author\":{\"name\":\"Joeri Hofstede\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#\\\/schema\\\/person\\\/3b50e6935852914b33d115caa22002cb\"},\"headline\":\"ASTM A578 \\\/ SA-578: Ultraschallpr\u00fcfung von Blechen und plattierten Blechen\",\"datePublished\":\"2026-11-04T08:32:58+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/\"},\"wordCount\":966,\"commentCount\":0,\"publisher\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/automated-phased-array-ut-clad-plate.jpg\",\"articleSection\":[\"Technische Bibliothek\"],\"inLanguage\":\"de\",\"potentialAction\":[{\"@type\":\"CommentAction\",\"name\":\"Comment\",\"target\":[\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#respond\"]}]},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/\",\"name\":\"ASTM A578 \\\/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/automated-phased-array-ut-clad-plate.jpg\",\"datePublished\":\"2026-11-04T08:32:58+00:00\",\"description\":\"ASTM A578 \\\/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#breadcrumb\"},\"inLanguage\":\"de\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#primaryimage\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/automated-phased-array-ut-clad-plate.jpg\",\"contentUrl\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/automated-phased-array-ut-clad-plate.jpg\",\"width\":1600,\"height\":900,\"caption\":\"Automatisierte Phased-Array-Ultraschallpr\u00fcfung der Bindung eines sprengplattierten Blechs bei Shockwave\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/astm-a578-ultraschallpruefung-plattierte-bleche\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"ASTM A578 \\\/ SA-578: Ultraschallpr\u00fcfung von Blechen und plattierten Blechen\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#website\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/\",\"name\":\"Shockwave\",\"description\":\"Shockwave Metalworking Technologies\",\"publisher\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#organization\"},\"alternateName\":\"Shockwave Metalworking Technologies\",\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"de\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#organization\",\"name\":\"Shockwave Metalworking Technologies BV\",\"alternateName\":\"Shockwave\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2025\\\/09\\\/logo-shockwave.png\",\"contentUrl\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/uploads\\\/2025\\\/09\\\/logo-shockwave.png\",\"width\":300,\"height\":343,\"caption\":\"Shockwave Metalworking Technologies BV\"},\"image\":{\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.linkedin.com\\\/company\\\/shockwave-metalworking-technologies-b-v\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/de\\\/#\\\/schema\\\/person\\\/3b50e6935852914b33d115caa22002cb\",\"name\":\"Joeri Hofstede\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/litespeed\\\/avatar\\\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938\",\"url\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/litespeed\\\/avatar\\\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938\",\"contentUrl\":\"https:\\\/\\\/shockwave-clad.com\\\/wp-content\\\/litespeed\\\/avatar\\\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938\",\"caption\":\"Joeri Hofstede\"},\"sameAs\":[\"https:\\\/\\\/shockwave-clad.com\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave","description":"ASTM A578 \/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/","og_locale":"de_DE","og_type":"article","og_title":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave","og_description":"ASTM A578 \/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.","og_url":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/","og_site_name":"Shockwave","article_published_time":"2026-11-04T08:32:58+00:00","og_image":[{"width":1600,"height":900,"url":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg","type":"image\/jpeg"}],"author":"Joeri Hofstede","twitter_card":"summary_large_image","twitter_misc":{"Verfasst von":"Joeri Hofstede","Gesch\u00e4tzte Lesezeit":"5\u00a0Minuten"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#article","isPartOf":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/"},"author":{"name":"Joeri Hofstede","@id":"https:\/\/shockwave-clad.com\/de\/#\/schema\/person\/3b50e6935852914b33d115caa22002cb"},"headline":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung von Blechen und plattierten Blechen","datePublished":"2026-11-04T08:32:58+00:00","mainEntityOfPage":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/"},"wordCount":966,"commentCount":0,"publisher":{"@id":"https:\/\/shockwave-clad.com\/de\/#organization"},"image":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#primaryimage"},"thumbnailUrl":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg","articleSection":["Technische Bibliothek"],"inLanguage":"de","potentialAction":[{"@type":"CommentAction","name":"Comment","target":["https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#respond"]}]},{"@type":"WebPage","@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/","url":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/","name":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung erkl\u00e4rt | Shockwave","isPartOf":{"@id":"https:\/\/shockwave-clad.com\/de\/#website"},"primaryImageOfPage":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#primaryimage"},"image":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#primaryimage"},"thumbnailUrl":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg","datePublished":"2026-11-04T08:32:58+00:00","description":"ASTM A578 \/ SA-578 erkl\u00e4rt: Senkrechteinschallung von Stahlblechen, Pr\u00fcfraster, Registrierung, Zul\u00e4ssigkeitsstufen A, B und C und Anwendung auf plattierte Bleche.","breadcrumb":{"@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#breadcrumb"},"inLanguage":"de","potentialAction":[{"@type":"ReadAction","target":["https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/"]}]},{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#primaryimage","url":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg","contentUrl":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2026\/10\/automated-phased-array-ut-clad-plate.jpg","width":1600,"height":900,"caption":"Automatisierte Phased-Array-Ultraschallpr\u00fcfung der Bindung eines sprengplattierten Blechs bei Shockwave"},{"@type":"BreadcrumbList","@id":"https:\/\/shockwave-clad.com\/de\/astm-a578-ultraschallpruefung-plattierte-bleche\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/shockwave-clad.com\/de\/"},{"@type":"ListItem","position":2,"name":"ASTM A578 \/ SA-578: Ultraschallpr\u00fcfung von Blechen und plattierten Blechen"}]},{"@type":"WebSite","@id":"https:\/\/shockwave-clad.com\/de\/#website","url":"https:\/\/shockwave-clad.com\/de\/","name":"Shockwave","description":"Shockwave Metalworking Technologies","publisher":{"@id":"https:\/\/shockwave-clad.com\/de\/#organization"},"alternateName":"Shockwave Metalworking Technologies","potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/shockwave-clad.com\/de\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"de"},{"@type":"Organization","@id":"https:\/\/shockwave-clad.com\/de\/#organization","name":"Shockwave Metalworking Technologies BV","alternateName":"Shockwave","url":"https:\/\/shockwave-clad.com\/de\/","logo":{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/shockwave-clad.com\/de\/#\/schema\/logo\/image\/","url":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2025\/09\/logo-shockwave.png","contentUrl":"https:\/\/shockwave-clad.com\/wp-content\/uploads\/2025\/09\/logo-shockwave.png","width":300,"height":343,"caption":"Shockwave Metalworking Technologies BV"},"image":{"@id":"https:\/\/shockwave-clad.com\/de\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.linkedin.com\/company\/shockwave-metalworking-technologies-b-v\/"]},{"@type":"Person","@id":"https:\/\/shockwave-clad.com\/de\/#\/schema\/person\/3b50e6935852914b33d115caa22002cb","name":"Joeri Hofstede","image":{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/shockwave-clad.com\/wp-content\/litespeed\/avatar\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938","url":"https:\/\/shockwave-clad.com\/wp-content\/litespeed\/avatar\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938","contentUrl":"https:\/\/shockwave-clad.com\/wp-content\/litespeed\/avatar\/c58d8285d33673a57f692e7219a419ee.jpg?ver=1793641938","caption":"Joeri Hofstede"},"sameAs":["https:\/\/shockwave-clad.com\/"]}]}},"_links":{"self":[{"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/posts\/5843","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/users\/3"}],"replies":[{"embeddable":true,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/comments?post=5843"}],"version-history":[{"count":2,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/posts\/5843\/revisions"}],"predecessor-version":[{"id":5944,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/posts\/5843\/revisions\/5944"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/media\/5834"}],"wp:attachment":[{"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/media?parent=5843"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/categories?post=5843"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/shockwave-clad.com\/de\/wp-json\/wp\/v2\/tags?post=5843"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}